Products Polypropylene concrete fiber Macro synthetic fiber Buy concrete fiber Applications Calculators About us Technical notes Contact Request a quote

Technical note

Fiber Reinforced Asphalt: What It Does, Dose and Tests

Steel drum roller compacting a fresh mat of fiber reinforced asphalt on a rural road at sunset

Fiber reinforced asphalt is a hot asphalt mix with a small dose of short fibers added at the plant, measured as a share of the mix mass. In mixes rich in binder, the fibers help hold the binder on the stone, so it does not drain off during storage and haul. In other mixes they can add resistance to cracking and rutting. However, that gain depends on your aggregate, binder and gradation, so a lab test on your own mix has to show it first. Our asphalt grade, PG AS-20, is a 20 mm fiber dosed at 0.05 to 0.3% of the mix weight.

What fiber does inside an asphalt mix

Fiber has two separate jobs in asphalt, and it helps to keep them apart. First, it stabilises the binder while the mix is still loose and hot. Second, it reinforces the layer after compaction.

Holding the binder in place

Stone matrix asphalt (SMA) is the classic case. An FHWA technical brief on stone matrix asphalt describes SMA as 70 to 80 percent coarse aggregate and 6 to 7 percent binder. Because it carries more binder than a dense-graded mix, it tends to drain down during silo storage and transport. As a result, producers add a small amount of fiber to reduce it: about 0.3 percent for cellulose and 0.3 to 0.4 percent for mineral fiber. The fiber network then holds the binder film on the stone until the roller has done its work.

Reinforcing the compacted layer

Fiber reinforced asphalt in a dense-graded mix is a different idea. Here the fibers spread through the layer and resist the growth of cracks. For example, researchers at Arizona State University summarised several studies on a blend of polypropylene and aramid fibers. In flexural and fracture tests, the fiber reinforced asphalt concrete resisted crack formation and crack growth better than the control mix. Its stiffness results also pointed to better rutting and fatigue resistance.

Results are not always one-sided, though. A lab study in Iran tested polypropylene fiber in an asphalt binder course. The fiber raised the strength of the mix and lowered its rutting potential. Yet the same fiber made the asphalt more sensitive to moisture. So one property can improve while another gets worse. That is why every claim about fiber needs a test on your mix.

What fiber does not do

Fiber is not a modified binder. Polymer-modified binder changes the binder itself, while fiber stabilises and reinforces the mixture. In fact, the FHWA brief notes that studies found polymer-modified binder used together with fiber improved durability and resistance to both rutting and cracking. So treat the two as partners, not substitutes. Also, fiber cannot rescue a weak base, poor compaction or the wrong gradation.

Where fiber reinforced asphalt makes sense

Fiber earns its place where a mix has a known weakness that a lab can measure. Typical cases include:

  • SMA and other gap-graded mixes with a high binder content, where drain-down is the main risk.

  • Surfaces under slow, heavy or channelised traffic, such as bus lanes, intersections and port aprons, where rutting is the concern.

  • Overlays on cracked or jointed bases, where the aim is to slow reflective cracks coming up from below.

On the other hand, fiber is not the only answer to drain-down. For example, FHWA reports pilot projects with fiberless SMA. In those, warm-mix technology and a lower production temperature kept drain-down in check without fibers. If drain-down is your only problem, compare that route as well.

Dosing fiber reinforced asphalt by mix weight

Asphalt is produced and sold by the tonne, so the fiber dose follows the mass of the mix. Compared to concrete, which we dose per cubic metre, that is a change of habit. PG AS-20 has a band of 0.05 to 0.3% by mass of total mix. Then the arithmetic is simple:

Point in the bandDose (% of mix mass)Fiber per tonne of mixAmount for a 2-tonne batch
Bottom0.05%0.5 kg1 kg
Low0.1%1 kg2 kg
Middle0.2%2 kg4 kg
Top0.3%3 kg6 kg

Before production starts, make sure the lab, the plant and the fiber supplier all use the same basis. A percentage of total mix is not the same as a percentage of binder weight, and mixing them up changes the dose many times over. Also, more fiber is not automatically better. Because of that, the lab evaluation sets where your mix sits in the band, and the plant then holds that dose.

Adding fiber at the asphalt plant

Fiber goes in at the plant, never on the road. For example, in a batch plant it goes into the pugmill. In a drum plant, however, it needs a feed point on the drum mixer. Either way, the feed rate follows the mass of mix, and the crew checks the mixing time during commissioning. The plant is where fiber reinforced asphalt succeeds or fails.

Asphalt paver laying a fresh black mat on a rural road on a clear day

A few plant habits keep the dose honest:

  • Weigh the fiber for each batch, or calibrate the feeder against the tonnage it serves.

  • Record the dose on the plant ticket next to the mix design number.

  • Store fiber dry and closed until use.

  • Look at the first loads at discharge. Clumps of fiber mean the feed point or the mixing time needs a change.

Temperature matters too. Polypropylene has a melting point of 160 to 170 °C, a nominal value for the base polymer. So compare that with your plant's mixing and discharge temperatures. Then ask the fiber maker how its fiber behaves at those temperatures, and confirm the answer in the trial. On site, the paver and crew method stay the same. Still, confirm the compaction temperature and rolling pattern on a trial section before the main job.

What to test before you specify fiber reinforced asphalt

Test the fiber mix against a control. Use the same aggregate, binder and gradation, so that the only difference is the fiber. Then run the tests that match the problem you want to solve.

  • Drain-down. ASTM D6390 measures how much binder drains from loose mix held at production temperatures. It applies in particular to porous asphalt and SMA. AASHTO T 305 covers the same property.

  • Rutting and moisture damage. The Hamburg wheel-track test (AASHTO T 324) rolls a loaded wheel over submerged specimens and records the rut depth.

  • Cracking. ASTM D8225, the indirect tensile cracking test at intermediate temperature, gives a cracking tolerance index for the mix.

  • Moisture sensitivity. Also run the moisture test your specification names. As the Iranian study shows, fiber can push this result the wrong way.

Row of road rollers and paving machines parked on a newly paved wet street

Write the pass criteria before the first sample goes in the oven. If the fiber mix beats the control on the property you care about and does not lose on the others, you have a case. If not, change the dose or drop the fiber.

What to ask a fiber supplier

Overall, the checks are the same ones a careful buyer uses for concrete. First, ask whether the polymer is virgin or recycled; our guide to virgin polypropylene fiber lists six checks before you buy. Next, ask how the supplier controls length, since the logic of polypropylene fiber length carries over from concrete. Then ask for a data sheet, a QC certificate with each batch and a sample big enough for the whole lab programme.

PG AS-20 for fiber reinforced asphalt uses the same 100% virgin polypropylene as our polypropylene concrete fibers. Polyguard runs an ISO 9001 quality system and its own laboratory, and every production batch has its own QC certificate. We also send a free sample for your trial, plus test reports for the method your specification names on request. The asphalt fiber page covers the grade in more detail. For samples and quotes, talk to us as your concrete fiber supplier, or start with how concrete fiber works if fiber is new to you.

Frequently Asked Questions

How much fiber goes into fiber reinforced asphalt?

The dose follows the mass of the mix. For PG AS-20 the band is 0.05 to 0.3% of total mix weight, which is 0.5 to 3 kg per tonne. A lab evaluation on your own mix sets where in the band you sit.

Does fiber replace polymer-modified binder?

No. Polymer-modified binder changes the binder itself, while fiber stabilises and reinforces the mixture. The two are often used together rather than one instead of the other.

Where is fiber added to an asphalt mix?

At the plant, never on the road: into the pugmill of a batch plant or through a feed point on a drum mixer. The feed rate follows the mass of mix, and the mixing time is checked during commissioning.

Which tests show whether fiber helps an asphalt mix?

Test the fiber mix against the same mix without fiber. Use drain-down (ASTM D6390 or AASHTO T 305) for SMA and porous mixes, the Hamburg wheel-track test for rutting, ASTM D8225 for cracking, and the moisture test your specification names.

Keep reading

Related notes